Vulcanizating agents dispersion UGB 810
Vulcanizating agents dispersion UGB 810
Details

Application     

  latex thread                     

Main components

  Sulphur,ZnO,accelerant,Antioxidant,dispersant.                                  

Characteristic data

Characteristics

Units

Values

Partical size

um

D50 5 

D90 9

Solid content

%

53

PH value


10±1

Recommend dosage


Material Name

Usage AmountKG

1. Natural latex per-vulcanized

Natural latex

100

30% potassium hydroxide solution

1.2

60% kaolin grinding liquid

25

Potassium oleate emulsion

0.5

Emulsified silicone oil

0.07

Vulcanizating agents dispersion UGB 810

6.2

2After per-vulcanized

Accelerator HB emulsion

0.05

 

Instruction

- Add natural latex (temperature 30-32), potassium hydroxide solution, stir while adding;
- Add kaolin grinding solution, stir and disperse evenly;
- Add the potassium oleate emulsion and stir well.

- Add the UGB 810, stir and disperse evenly, stir at a slow speed for 6-8 hours; After the swelling rate reaches the standard, the pre-vulcanization is completed.

-Add the accelerator HB emulsion, stir evenly, and send to the homogenizer for homogenization.

-After homogenization, send the latex to the cooling tank to cool to 17-19for use.

Remarks

Be sure to stir well before use to avoid affecting material performance.